2 Painting Wrongs Don’t Make a Right

Friday, March 21, 2014

Comment | More

There’s a rule that paint inspectors live by: When you look at the exterior concrete walls of a high-rise condo or apartment building, don’t assume that the paint is planning to stay there.

MPI Peeling Paint
Photos: MPI

You have one chance to get the initial new-construction high-rise paint job right. Bad decisions at that stage won't hide for long.

The paint may look intact to the naked eye, but there may be little or no adhesion between the coating and the underlying wall. Any stress applied to the paint film—such as applying a repaint coat—may cause immediate and dramatic failure.

That’s because the same error gets made again and again at the new-construction phase. And if it’s not caught and corrected at the first repaint, the price of fixing the problem can escalate dramatically.

That’s what this paint inspector saw when investigating a problem on an 18-story high rise.

The Case of the High-Rise Repaint

It had been nine years since the initial construction and paint job, and it was time to freshen up the finish. The owner awarded the bid to a qualified painting contractor whose bid had noted bubbles and blisters in the existing paint film that the contractor believed were the result of high moisture content in the concrete.

The bid stated that the contractor would remove all bubbles and areas of weak adhesion and that if the bubbles reappeared, “they would be repaired once the cause is identified.”

This type of language alone should have thrown red flags all over the bid and the project.

The first rule of maintenance repainting is: When the existing film exhibits obvious evidence of failure, don’t write the repaint spec or even think about starting the job until the cause of the existing failure is determined AND rectified.

Otherwise, there’s a very good chance that whatever caused the initial coating to fail will cause the repaint coat to fail, and you’ll have thrown a lot of money down the drain.

More Flags

Nevertheless, the project went forward. The paint supplier and product were selected, and a coating approved under MPI #40 Latex, Exterior, High Build was applied at 10-12 mils. The manufacturer’s five-year warranty required it to do a site review to evaluate the surface before painting.

The manufacturer’s reps submitted multiple reports that noted the same blisters and adhesion failures, but they didn’t contact the owner to discuss the problem and how it could impact the warranty.

Another red flag.

The contractor then proceeded with the job, prepping the surface with a thorough power wash to remove dirt and contaminants, and then applying the specified coating.

When several tenants complained that the new paint visible from their balconies showed signs of significant bubbling and blistering, this paint inspector was called in.

What the Inspector Saw

The inspector looked at two balconies, noted the paint bubbles and blisters, cut them in half, and found that the edges could easily be peeled off in sheets down to the bare concrete surface.

ASTM D3359 testing

ASTM D3359 adhesion testing easily removed the paint to bare concrete. The actual project is not pictured.

On the back of the sheets of paint were telltale signs of concrete dust. Applying adhesion tape as described in ASTM D3359 elicited the same results. Both the original and new coating were easily removed down to bare concrete, again with substantial evidence of dust and contaminants on the back of the paint film.

The bare concrete also showed considerable dust and the weak, thin cover called laitance. These were poured-in-place walls; with poured-in-place, the vibration required to consolidate the concrete can push water and fine particles to the surface, creating laitance. Laitance must be removed during initial surface preparation, or failures like this can occur.

Sacking Havoc ... Again

It was also apparent that the concrete had been sacked during original construction to fill bug holes and surface imperfections.

The considerable dust on the bare concrete surface suggested that the sacking material had deteriorated over time.

In our experience, if you peel off the coating and see a lot of dust stuck to the back of the film—and when you touch the bare substrate underneath and get concrete dust all over your hands—you’ve got either a sacking or laitance problem, or both.

This is by far the most common failure we find on exterior high-rise concrete walls.

Sacking dust

The inspector's fingers are coated with concrete dust from the bare substrate under the coating. Right: Sacking dust on the back of the paint film.

It begins thus: The same vibration that leads to laitance can cause air bubbles to be trapped at the form face, resulting in the tiny voids or holes in the concrete surface we call bugholes. Most architects and owners consider these holes unsightly and request that sacking be applied to fill them.

We understand the desire for an aesthetically pleasing wall surface, but keep in mind that it takes a great deal of skill to apply sacking material properly. All too often, sacking creates a weak layer of poorly adhered concrete, and failure to remove these weak layers before the initial paint job can lead to failures like the one described here.

Painting Over Mistakes

The inspector also noted hard edges in the existing film that had been overcoated with the repaint finish, which suggests that the painter had likewise seen the blisters, picked at the failed areas, stripped off the blistered paint just as easily as the inspector had, and then simply coated over the area.

Blisters

Note the hard edges above and to the right of the blister. Non-adhering paint was apparently stripped to the bare concrete, and a new coat was applied over it.

This is not a recommended protocol. If you, as the painter, can peel the blistered film off the surface in sheets down to the bare concrete, stop what you’re doing and inform the owner. Continuing the job is the painter’s version of walking in the Valley of the Shadow of Death.

It is unclear in this case whether the contractor failed to report the problems he saw—or if he had reported the problems to the owner, and the owner had chosen to ignore them.

The Inspector’s Diagnosis

The inspector gave this report to the owner.

The problem appeared to have started when, before paint application to the new construction, the wall surfaces were not cleaned properly, so the coating was applied over poor-quality sacking and laitance residue. These contaminants created a barrier that impeded adhesion between the substrate and the coating.

The lack of adhesion was evidenced by the bubbles and blisters present when the repaint job was bid. When the new coating was applied over the existing film, the stresses exerted on the existing film by the new film as it shrank in the curing process led to the widespread bubbles and blisters the tenants were now complaining about.

So now, the owner had what was essentially a coating time bomb on his hands. The lack of adhesion was almost certainly widespread over the building — not just on the balconies the inspector examined — so the blistering was likely to grow as freeze/thaw and other stresses are exerted on the coating.

How to Fix the Problem

The inspector recommended that:

  • The coatings in the poorly adhering areas be removed in their entirety;
  • The surface be cleaned to remove all dust and laitance material; and
  • The affected balconies recoated edge to edge.
Paint and Power Wash

Note the two sets of scaffolding. Painters are power washing up above, while other painters paint below. A wall should never be power-washed and painted on the same day.

Hand and power tools can be suitable for coating removal where the adhesion is so poor. If pressure washing is used either for paint removal or to clean the surface of dust and laitance, remember that you are wetting the concrete, which can create a new problem for coating adhesion.

Moisture meter readings should be taken in the same area before and after power washing to assure that the concrete moisture level is back to its original state before coating application. Under no circumstances should the coating be applied the same day as the power washing.

And the coating manufacturer’s warranty? We assume it will not be forthcoming, since the coating performed properly. It adhered perfectly to the existing film, which is essentially what the paint manufacturer is warranting.

(When both the new and the old coating peel from the surface, the warranty is highly in doubt.)

In dollars and cents, we estimate the total cost for the job would now be $250,000, which is quite a few ticks above the $100,000 the owner originally planned.

Lessons Learned

1: Don’t Create the Problem In the First Place

The first “wrong” in this case was committed at new construction. The painting contractor performed insufficient or non-existent surface prep.

And it appears that no professional coating inspection was used. Paint inspectors are keenly aware of the need to remove all dust and contaminants from the surface before painting, so hiring an inspector for the job could have assured proper prep.

Bug holes

No sacking remains in the bug holes on the left side. It came off with the paint film.

Furthermore, if the painter is facing a newly sacked concrete wall, doing a test patch is an absolute must. Apply a coat of the selected material over a sacked area, allow it to cure, and then do an adhesion test.

Most often, you’ll either get a rating 5A (perfect adhesion) or 0A (coating peels right off with a load of fine concrete dust on the back).

So consider this: A $100,000 paint job can fail because no one spent $35 on a role of adhesion test tape.

2: Don’t Just Paint Over It

As we said in the beginning: Always determine the cause of failure before writing the repaint spec, let alone doing the job. It appears that this owner and contractor allowed work to start and continue despite knowing that there could be an escalating problem.

On the other hand, a professional paint inspector could have been called in once the first blisters were noted and had the problem diagnosed in less than an hour, as follows:

  • 1 to 1:05 p.m.: Inspector pulls up to building, greets the owner, and exchanges pleasantries.
  • 1:05 to 1:10 p.m.: Inspector takes elevator to the ninth floor, knocks on condo door, and is escorted to the balcony.
  • 1:10 to 1:20 p.m.: Inspector leans over, sees blisters in the coating, cuts a few in half, and removes sheets of paint like they were wallpaper. Inspector pulls out adhesion tape test kit, makes the required cuts, applies and pulls off adhesion tape, finds zero adhesion and a load of dust on the back of the tape.
  • 1:20 to 1:25 p.m.: Inspector goes back down in elevator.
  • 1:25 to 1:55 p.m.: Inspector explains to owner why his paint is peeling and what steps should be taken before applying a new coat.

It’s not always this simple, but often enough, it is.

Penny Wise, Coating Foolish

After seeing so many failures like this, we find it interesting that contractors, owners, engineers, and architects can spend a year or more developing specifications and bid documents; let paint jobs for $100,000 or more; and then hesitate to invest roughly $5,000 on coating inspection to assure the paint is going to perform as expected.

It’s a shame, because in new construction, you’ve got all the tools to do the job right the first time and assure maximum life expectancy from the applied coatings.

But in repaint work, all of the parties—the owner, the paint manufacturer’s rep, and the contractor—are required to walk in and fix what could be the careless and costly oversights of the team that came before them.

Editor's Note: This article was written by PQA Inspector Clayton Des Roches and is reprinted with permission from the MPI (Master Painters Institute) newsletter. MPI content describes best practices for commercial, institutional, and light industrial painting.

   

Tagged categories: Coating inspection; Commercial contractors; Condominiums/High-Rise Residential; Good Technical Practice; Laitance; Maintenance coating work; Master Painters Institute (MPI); Paint application; Paint defects; Surface preparation

Comment Join the Conversation:

Sign in to our community to add your comments.


 
 
 

Technology Publishing Co., 1501 Reedsdale Street, Suite 2008, Pittsburgh, PA 15233

TEL 1-412-431-8300  • FAX  1-412-431-5428  •  EMAIL webmaster@paintsquare.com


The Technology Publishing Network

PaintSquare the Journal of Protective Coatings & Linings Paint BidTracker

 
EXPLORE:      JPCL   |   PaintSquare News   |   Interact   |   Buying Guides   |   Webinars   |   Resources   |   Classifieds
REGISTER AND SUBSCRIBE:      Free PaintSquare Registration   |   Subscribe to JPCL   |   Subscribe to PaintSquare News
MORE:      About PaintSquare.com   |   Privacy Policy   |   Terms & Conditions   |   Support   |   Site Map   |   Search   |   Contact Us